LAMPIRAN 3 HASIL PENGUJIAN SEM-EDX
1. PVB 2
Universitas Sumatera Utara
Spectrum processing : Peaks possibly omitted : 1.500, 1.730, 12.790 keV
Processing option : All elements analyzed Normalised Number of iterations = 3
Standard : C CaCO3 1-Jun-1999 12:00 AM
O SiO2 1-Jun-1999 12:00 AM Fe Fe 1-Jun-1999 12:00 AM
Co Co 1-Jun-1999 12:00 AM Nd NdF3 1-Jun-1999 12:00 AM
Element Weight
Atomic C K
8.84 33.65
O K 2.03
5.81 Fe K
60.19 49.26
Co K 4.60
3.57 Nd L
24.33 7.71
Totals 100.00
Universitas Sumatera Utara
Spectrum processing : No peaks omitted
Processing option : All elements analyzed Normalised Number of iterations = 3
Standard : C CaCO3 1-Jun-1999 12:00 AM
O SiO2 1-Jun-1999 12:00 AM Fe Fe 1-Jun-1999 12:00 AM
Co Co 1-Jun-1999 12:00 AM Nd NdF3 1-Jun-1999 12:00 AM
Element Weight
Atomic C K
6.76 29.21
O K 0.47
1.54 Fe K
59.26 55.06
Co K 4.11
3.62 Nd L
29.39 10.57
Totals 100.00
Universitas Sumatera Utara
Spectrum processing : No peaks omitted
Processing option : All elements analyzed Normalised Number of iterations = 2
Standard : C CaCO3 1-Jun-1999 12:00 AM
O SiO2 1-Jun-1999 12:00 AM Fe Fe 1-Jun-1999 12:00 AM
Co Co 1-Jun-1999 12:00 AM Nd NdF3 1-Jun-1999 12:00 AM
Element Weight
Atomic C K
22.42 60.64
O K 2.65
5.39 Fe K
44.62 25.96
Co K 3.64
2.01 Nd L
26.67 6.01
Totals 100.00
Universitas Sumatera Utara
2. PVB 4
Universitas Sumatera Utara
Spectrum processing : Peaks possibly omitted : 1.497, 12.780 keV
Processing option : All elements analyzed Normalised Number of iterations = 3
Standard : C CaCO3 1-Jun-1999 12:00 AM
O SiO2 1-Jun-1999 12:00 AM Fe Fe 1-Jun-1999 12:00 AM
Co Co 1-Jun-1999 12:00 AM Zn Zn 1-Jun-1999 12:00 AM
Nd NdF3 1-Jun-1999 12:00 AM
Element Weight
Atomic C K
7.43 29.51
O K 2.15
6.42 Fe K
60.83 51.95
Co K 4.90
3.96 Zn K
-0.03 -0.02
Nd L 24.72
8.17 Totals
100.00
Universitas Sumatera Utara
Spectrum processing : Peak possibly omitted : 3.317 keV
Processing option : All elements analyzed Normalised Number of iterations = 5
Standard : C CaCO3 1-Jun-1999 12:00 AM
O SiO2 1-Jun-1999 12:00 AM Si SiO2 1-Jun-1999 12:00 AM
Cl KCl 1-Jun-1999 12:00 AM Fe Fe 1-Jun-1999 12:00 AM
Co Co 1-Jun-1999 12:00 AM Nd NdF3 1-Jun-1999 12:00 AM
Element Weight
Atomic C K
65.92 81.26
O K 15.85
14.67 Si K
0.10 0.05
Cl K 0.23
0.09
Universitas Sumatera Utara
Fe K 11.94
3.17 Co K
0.97 0.24
Nd L 4.99
0.51 Totals
100.00
Universitas Sumatera Utara
Spectrum processing : Peaks possibly omitted : 1.740, 3.310 keV
Processing option : All elements analyzed Normalised Number of iterations = 4
Standard : C CaCO3 1-Jun-1999 12:00 AM
O SiO2 1-Jun-1999 12:00 AMFe Fe 1-Jun-1999 12:00 AM Co Co 1-Jun-1999 12:00 AM
Nd NdF3 1-Jun-1999 12:00 AM
Element Weight
Atomic C K
66.67 82.63
O K 14.20
13.22 Fe K
12.51 3.34
Co K 0.89
0.23
Nd L 5.73
0.59
Totals 100.00
Universitas Sumatera Utara
LAMPIRAN 4 DATA HASIL VSM
1. PVB 2